Film/coating

Conditions

OP (cc × µm/m2/day)

Reference

Pectina

0% RH, 23˚C

1000

[4]

Pectina

50% RH, 23˚C

2400

[4]

Pectina

80% RH, 23˚C

32,000

[4]

Pectina + 10% nanoclay

0% RH, 23˚C

600

[4]

Pectina + 10% nanoclay

50% RH, 23˚C

1200

[4]

Pectina + 10% nanoclay

80% RH, 23˚C

18,300

[4]

Pectina + 20% nanoclay

0% RH, 23˚C

400

[4]

Pectina + 20% nanoclay

50% RH, 23˚C

700

[4]

Pectina + 20% nanoclay

80% RH, 23˚C

11,300

[4]

Pectina + 30% nanoclay

0% RH, 23˚C

1400

[4]

Pectina + 30% nanoclay

50% RH, 23˚C

2600

[4]

Pectina + 30% nanoclay

80% RH, 23˚C

6400

[4]

Chitosan

80% RH, 23˚C

9800

[18]

Chitosan + 17% nanoclay

80% RH, 23˚C

4600

[18]

Chitosan + 50% nanoclay

80% RH, 23˚C

1900

[18]

Chitosan + 67% nanoclay

80% RH, 23˚C

1200

[18]

Chitosan crosslinked

80% RH, 23˚C

980

[17]

Chitosan crosslinked + 50% nanoclay

80% RH, 23˚C

280

[17]

CNFb bleached softwood

80% RH, 23˚C

5200

[35]

CNFb bleached hardwood

80% RH, 23˚C

2900

[35]

PVA-CNF

0% RH, 23˚C

0.5

[36]

PVA-CNF

90% RH, 23˚C

6790

[36]

PVA-CNF + 50% nanoclay

0% RH, 23˚C

0.5

[36]

PVA-CNF + 50% nanoclay

90% RH, 23˚C

190

[36]

CNF bleach birch pulp

0% RH, 23˚C

<1

[39]

CNF bleach birch pulp

50% RH, 23˚C

30

[39]

CNF bleach birch pulp

80% RH, 23˚C

800

[39]

CNFa bleach birch pulp

0% RH, 23˚C

3

[39]

CNFa bleach birch pulp

50% RH, 23˚C

1700

[39]

CNFa bleach birch pulp

80% RH, 23˚C

15,500

[39]

CNF bleach birch pulp (heat treated)

0% RH, 23˚C

<1

[39]

CNF bleach birch pulp (heat treated)

50% RH, 23˚C

2

[39]

CNF bleach birch pulp (heat treated)

80% RH, 23˚C

300

[39]

PVA

90% RH, 23˚C

45,000

[48]

CNF-PVA

90% RH, 23˚C

50,000

[48]

Epoxy-CNF-PVA

90% RH, 23˚C

48,000

[48]